Short Shots in Injection Molding: Causes and How to Fix Them
A short shot is one of the common defects found in plastic injection molding. It occurs when molten plastic does not completely fill the mold cavity, leaving part of the molded component missing or incompletely formed.
The defect may appear as a missing corner, an unfinished edge, an incomplete rib or a partially formed section.

Short shots can make a component unusable, especially when the missing material affects assembly, structural strength or product appearance.
Understanding why incomplete filling occurs is essential for maintaining stable production and reducing material waste.
This article explains the main causes of short shots in injection molding and practical methods manufacturers can use to prevent them.
1. What Is a Short Shot in Injection Molding?
A short shot occurs when the molten plastic stops flowing before the mold cavity is completely filled.
As a result, the finished part does not fully match the intended shape.
Typical signs include:
- Missing material at the end of a flow path.
- Incomplete ribs, thin walls or corners.
- Partially formed bosses or small structural features.
- Uneven or unfinished edges.
- A component that does not match the intended CAD geometry.
Short shots should not be confused with flash.
A short shot occurs when insufficient plastic fills the cavity, while flash occurs when excess plastic escapes through a gap in the mold.
2. Common Causes of Short Shots
Short shots can result from insufficient material flow, excessive flow resistance, trapped air or unsuitable molding conditions.
| Cause | Explanation | Possible Solution |
|
Insufficient injection volume |
Not enough molten plastic enters the cavity. |
Review shot size and injection volume. |
|
Low injection pressure |
The melt may not have enough pressure to reach the end of the cavity. |
Review injection pressure and machine capacity. |
|
Low melt temperature |
Plastic becomes too viscous and flows less easily. |
Verify the recommended material processing temperature. |
|
Low mold temperature |
The melt cools too quickly before filling the cavity. |
Review mold temperature and cooling balance. |
|
Blocked or restricted gate |
The gate limits the amount of material entering the cavity. |
Inspect the gate and runner system. |
|
Poor venting |
Trapped air can resist incoming melt flow. |
Inspect and improve mold venting. |
|
Excessive flow resistance |
Thin walls or long flow paths make filling difficult. |
Review part geometry, gate position and wall thickness. |
|
Material feeding problems |
Inconsistent material supply can reduce the available shot volume. |
Check the hopper, feeding system and material preparation. |
3. How Material Properties Affect Filling
Different plastic materials behave differently during injection molding.
Some materials flow more easily under suitable processing conditions, while others require more careful control of temperature, pressure and mold design.
Material viscosity, additives, fillers and moisture condition can all influence filling behavior.
For example:

ABS
Flow behavior varies by grade and can be affected by processing temperature and part geometry.

PP
Often offers good flow characteristics, although thin sections and long flow paths still require appropriate design.

PC
Processing conditions and drying requirements need careful attention.

PA
Moisture condition and grade selection can affect molding consistency.
Material selection should be based on the application and the actual grade's technical data rather than assuming that one resin family always fills better than another.
4. How to Fix Short Shots in Injection Molding
When a short shot occurs, manufacturers should identify the reason before making process adjustments.
1. Check the injection volume
Confirm that the machine is supplying enough material for the part, runner and required process cushion.
An insufficient shot size can prevent the cavity from filling completely.
2. Review injection pressure and speed
If pressure is insufficient, the melt may not reach the end of the cavity.
A suitable injection speed profile may also help maintain flow through thin sections.
However, increasing pressure or speed without checking other conditions can introduce additional defects.
3. Verify melt and mold temperatures
If the material cools too quickly, its flow may become restricted before the cavity is filled.
Check actual material and mold temperatures against the resin supplier's recommendations.
Avoid excessive temperatures that could cause material degradation.
4. Inspect the gate and runner system
A gate that is too small, partially blocked or poorly positioned can restrict material flow.
Check for contamination, wear and other restrictions in the runner and gate system.
5. Improve mold venting
Air trapped inside the cavity can prevent molten plastic from reaching certain areas.
Inspect the venting locations, especially near the end of the flow path and areas where filling is incomplete.
6. Review the part design
Thin walls, narrow channels and long flow paths can make filling more difficult.
Where product design allows, review wall thickness, gate position and geometry transitions with the mold designer.

5. Short Shot vs. Other Injection Molding Defects
Several molding defects can affect the appearance of a plastic component, but their causes are different.
|
Defect |
Main Appearance |
Typical Cause |
|---|---|---|
|
Short shot |
Missing or incomplete material |
Insufficient filling or restricted flow |
|
Flash |
Thin excess plastic around edges or parting lines |
Excessive cavity pressure or poor mold closing/sealing |
|
Sink marks |
Local depressions on the surface |
Uneven shrinkage, insufficient packing or thick sections |
|
Weld lines |
Visible lines where separate melt fronts meet |
Flow fronts joining during filling |
|
Burn marks |
Dark or discolored areas |
Trapped air or excessive material temperature |
|
Warpage |
Part bends or twists after molding |
Uneven shrinkage and cooling |
Correctly identifying the defect is important because the solutions are not interchangeable.
6. A Practical Troubleshooting Checklist
When a short shot is found during production, follow a structured inspection process.
|
Step |
Inspection Item |
What to Check |
|---|---|---|
|
1 |
Defect location |
Identify exactly where the part is incomplete. |
|
2 |
Material supply |
Check whether the correct amount of material is available. |
|
3 |
Machine settings |
Review shot size, pressure, speed and filling time. |
|
4 |
Material temperature |
Verify the actual melt temperature and material condition. |
|
5 |
Mold temperature |
Check temperature distribution and cooling conditions. |
|
6 |
Gate and runner |
Inspect for blockage or excessive flow restriction. |
|
7 |
Mold venting |
Check whether trapped air is preventing complete filling. |
|
8 |
Part geometry |
Review thin sections, long flow paths and design limitations. |
|
9 |
Trial verification |
Make controlled adjustments and compare the resulting parts. |
Changing several process parameters at the same time makes it difficult to identify the actual cause.
A controlled troubleshooting approach is more reliable.

7. How to Prevent Short Shots During Mass Production
Preventing short shots requires attention to both mold development and production control.
Before mass production:
- Review the part design for difficult-to-fill areas.
- Confirm suitable gate and runner dimensions.
- Check mold venting.
- Verify material specifications and preparation requirements.
- Conduct mold trials and inspect the complete cavity filling result.
During production:
- Maintain stable machine settings.
- Monitor material feeding and drying where required.
- Keep the gate, runner and venting system clean.
- Record process adjustments and inspection results.
- Investigate recurring incomplete filling rather than relying on temporary parameter changes.
A stable process should produce complete parts consistently, not just one acceptable sample.
How JIEJIN PLASTIC Supports Injection Molding Projects
JIEJIN PLASTIC provides custom plastic product development, mold manufacturing, 3D printing and injection molding production.
Our engineering team can review part geometry and discuss moldability, material selection, gate positioning and manufacturing considerations during product development.
For new projects, early design review can help identify difficult-to-fill features before the mold is manufactured.
If you are experiencing short shots or other injection molding issues, sharing the part drawing, material information, photos of the defect and relevant production details can help establish the next steps for technical evaluation.




Looking for a Reliable Plastic Manufacturing Partner?
Custom Manufacturing Solutions by JIEJIN PLASTIC
Plastic Injection Molding · Custom Plastic Parts · 3D Printing · Packaging Solutions
Frequently Asked Questions
Q1: What is a short shot in injection molding?
-
A short shot occurs when molten plastic does not completely fill the mold cavity, resulting in a partially formed or incomplete plastic component.
Q2: What is the most common cause of short shots?
-
Possible causes include insufficient injection volume, low injection pressure, unsuitable material temperature, restricted gates, poor venting and difficult part geometry. The actual cause should be identified through inspection.
Q3: Can increasing injection pressure solve short shots?
-
It may help when insufficient pressure is the cause. However, other factors such as blocked gates, trapped air and low material temperature may require different solutions.
Q4: Can mold design cause short shots?
-
Yes. Gate location, runner dimensions, venting and cavity geometry can all influence how molten plastic fills the mold.
Q5: Are short shots and flash the same defect?
-
No. A short shot means the cavity is not completely filled. Flash is excess plastic escaping from the mold cavity, usually near the parting line or other gaps.